Preparing a ceramic tube for a swagelok

Scritto da Robert Greenyer on .

For those needing to grind/machine the ends of sintered ceramic tubing, Bob Higgins has some advice...

"Here is a photo of machining the end of the alumina tube to 3/8" OD to accept the Swagelok nut and ferrules.  I put a piece of heatshrink tubing loosely around the tube and clamped it gently in the 3-jaw chuck in my lathe.  For a turning tool, I mounted a Dremel tool on the tool-post and in the Dremel was a diamond drum that was 1/4" diameter and 0.5" long like this one from eBay:

Diamond cutter

I made cuts ~0.0005" (12.5 microns) in each pass and cut 0.7" from the end of the tube.  The cutting was done dry with the lathe and Dremel tool turning in opposite directions.  Cutting slowly did not generate much heat and the diamond drum worked fine for all 3 tubes I machined (no indication that it became worn out)."

Add comment


Security code
Refresh

Comments   

 
0 #6 priscillawheuer 2024-09-09 10:48
Lost Mary BM5000 Flavors provide an exceptional vaping experience with a variety of bold e-liquid options. This sleek, disposable device features a long-lasting battery, delivering smooth, flavorful puffs for extended enjoyment.
Quote
 
 
0 #5 janet 2020-06-05 00:36
Heyy :) Nice blog, I must say that I really like to read here.

My snap is: janetisbored if you want to add me :) F 21
Quote
 
 
0 #4 allah sprüche 2017-03-13 06:18
Appreciating the dedication you put into your blog and
in depth information you provide. It's nice to come
across a blog every once in a while that isn't the same outdated
rehashed information. Fantastic read! I've saved your site and I'm including your RSS feeds to
my Google account.
Quote
 
 
0 #3 AlanG 2015-07-20 16:35
One detail I found necessary if a Swagelok pass-through is used, as for a core thermocouple or electrode. The ceramic tubes are made by extrusion and the inner and outer diameters are not perfectly concentric as manufactured.

The grinding process offers an opportunity to correct this. Using a live center tool when machining the end of the tube will make the ground outer surface concentric with the bore. The Swagelok pass-through hole will then line up with the bore so that the thermocouple sheath or electrode doesn't bind.
Quote
 
 
0 #2 Alan Smith 2015-07-19 10:16
Good information - many thanks. I have done quite a bit of machining using diamond tooling on both glass and ceramics, but always using water-flushed cutting surfaces. My main comment is to be very careful about the dust thrown off during dry machining materials like this. Aluminium oxide is a potentially serious lung irritant with long term consequences for health. Doing this a few times ordinary care and dust masks is probably enough, but I would prefer to use a fresh-air face mask and clean up the area afterward with a damp or oily cloth that gets binned afterwards.
Quote
 
 
0 #1 Ecco 2015-07-19 10:00
Coincidentally, a few days ago I tried searching the net for information on machining alumina ceramic tubes. Turns out it's not an easy task to do at all. Diamond bits are a must and the job should be preferably done with plenty of cooling and high lathe speeds.

I guess it must be easier if one only needs to grind the surface a bit, though.
Quote
 

Here is your generous contributions so far towards our $500,000 target, thanks everyone! : $45,020   Please Donate
See the current state of our booked costs here